Guide

Mechanised pipeline welding with an orbital carriage: Böhler pipeRunner guide

November 14, 2026 , Jarosław Kołaski

In mechanised pipeline welding with an orbital carriage, you weld the root and hot pass by hand. The carriage travels on a band around the pipe and lays the fill and cap passes. Böhler pipeRunner is that kind of carriage, also called a welding bug. It weighs 14 kg, welds pipe from 8 in upwards with flux-cored wire and stores up to 11 passes in one program. This guide takes you from choosing the kit, through joint preparation and parameters, to procedure qualification and purchase cost.

Our figures come from two sources. The first is data from voestalpine Böhler Welding. The second is the first pipeRunner trial in Poland, which we ran with a customer and the manufacturer. The pipe was 24 in (Ø610 mm) with a 17.5 mm wall, in L485ME steel. Where the manufacturer does not publish a figure, we say so in the text.

You can also watch the whole trial on our YouTube channel. The narrated video runs for 10 minutes 20 seconds.

Böhler pipeRunner in 6 numbers

ParameterValue
Carriage weight without spool14 kg
Smallest pipe diameter8 in (219.1 mm)
Travel speed0 to 1.6 m/min
Torch oscillation width0 to 60 mm
Passes in one programup to 11
Manufacturer's trial on 36 in x 15 mm pipe66 minutes per joint instead of 109

Who this guide is for

  • You run a site or a fabrication shop and want to know whether mechanising the fill passes will cut joint time.
  • You are a welding engineer or welding coordinator and you are preparing a WPS for flux-cored wire on a carriage.
  • You are an operator and want to see, step by step, what working with the carriage looks like.

You will find the price, kit contents and enquiry form on our orbital MIG/MAG pipe welding: Böhler pipeRunner page. See also the product page with price and lead time. Here we focus on how to weld with the system.

How the pipeRunner carriage and the hybrid method work

Böhler pipeRunner is a mechanised MIG/MAG carriage. It travels on a band fitted to the pipe next to the joint and guides the torch along the groove. The manufacturer designed it for uphill welding with flux-cored wire, that is, for the fill and cap passes. In the US this set-up is called bug-and-band welding, and the processes are SMAW (111), GTAW (141) and FCAW (136).

The 4 parts of the system

  • Guide band. A band of austenitic spring steel, made for one nominal pipe diameter. Spring-loaded stand-offs and a locking lever hold it on the pipe and compensate for ovality.
  • Carriage. An aluminium frame with 4 handles, brushless DC drives and a 5 kg spool on board. The torch has 65 mm of horizontal travel and 30 mm of vertical travel. It tilts by ±25° and oscillates up to 60 mm.
  • Power source. TERRA 400 PRM with the RC 100 MP remote control, 340 A at 100% duty cycle.
  • Program. Up to 11 passes, each with its own settings. You build the program in a PC application and adjust the settings from the remote control while welding.

Who welds which pass in the hybrid method

PassProcessWho weldsDirection
Root passcellulosic electrode (111) or TIG (141)welderdownhill with a cellulosic electrode
Hot passcellulosic electrode (111); for stainless steels and clad pipe as per the WPSwelderdownhill with a cellulosic electrode
Fill passesgas-shielded flux-cored wire (136)operator with pipeRunneruphill, from 6 o'clock to 12 o'clock
Cap passgas-shielded flux-cored wire (136)operator with pipeRunneruphill, with wider oscillation

You weld each half of the pipe separately. The carriage starts at the bottom, at 6 o'clock, and finishes at the top, at 12 o'clock. You weld the second half with the same carriage in the opposite direction, because the drive works both ways.

Why flux-cored wire, welded uphill

Rutile flux-cored wire forms a fast-freezing slag that supports the weld pool in the vertical position. That lets you weld uphill with oscillation and fuse into both sidewalls of the groove. Böhler pairs pipeRunner with seamless diamondspark RC-Pipe wires. Their classification carries the H4 designation, which means up to 4 ml of diffusible hydrogen per 100 g of weld metal. According to the manufacturer, the seamless design does not absorb moisture in storage.

What the pipeRunner kit consists of

Besides the carriage you need a band for your diameter, a power source, cables, wire and gas. The table shows an example kit with Böhler Welding part numbers.

ItemPart numberWhat it doesWhat to watch out for
pipeRunner carriage73.51.001travel on the band, oscillation and wire feed14 kg without spool, frame with 4 handles
Carriage remote control73.52.101controls the carriage at the jointthe operator holds it at all times
Carriage power supply, 230 V73.52.102powers the drives and the controlsneeds a 230 V supply
ABIMIG MT 305 machine torch, 0.75 mas per quotedelivers wire and gas to the groovethe contact tip and gas nozzle are the parts you replace most often
Guide band73.51.009 (14 in), 73.51.007 (24 in)track for the carriageone band per nominal diameter
TERRA 400 PRM power source55.13.011welding current from 3 to 400 A3 x 400 V supply, 30 A fuse, can run from a generator
RC 100 MP remote control for the power source71.02.209voltage adjustment at the jointdesigned for work on pipeline sites
CAN bus cable, 25 mas per quotecommunication between carriage and power sourceprotect the connectors from mud and crushing
Cable package 2 x 70 mm², 20 mas per quotewelding currentthe 20 m length limits how far the power source can be from the joint
diamondspark RC-Pipe flux-cored wire, 1.2 mmby steel gradefill and cap passesthe 5 kg spool rides on the carriage
M21 shielding gasnot applicablearc shielding15 to 25 l/min, a tent is needed on site
FOX CEL and FOX CEL 80-P cellulosic electrodesby diameterroot and hot passused by the welder, not the carriage

The manufacturer supplies the carriage in a case for transport and storage. The case has a pressure equalisation valve for air freight.

The price on the product page covers the base configuration. Your quote lists what it includes, and this may differ from the table above. We match the bands to your diameters, and the power source, torch and wire to your material and wall thickness. You will find the current list in the configuration section of the system page.

Böhler pipeRunner technical data

All values come from voestalpine Böhler Welding data.

Carriage

ParameterValue
Weight without spool14 kg
Dimensions480 x 400 x 260 mm
Pipe diameterfrom 8 in (219.1 mm); the manufacturer gives no upper limit
Travel speed0 to 1.6 m/min
Oscillation width0 to 60 mm
Oscillation speed0 to 350 cm/min
Horizontal torch travel65 mm
Vertical torch travel30 mm
Torch tilt±25°
Wire diameter1.0 to 1.6 mm
Wire feed speedup to 19 m/min
Current rating300 A at 100% duty cycle (CO2)
Passes per programup to 11
Travel directionclockwise and anticlockwise
Drivesbrushless DC motors
Wire spool5 kg
ProgrammingPC application; a ruggedised tablet is an option
Name variants you may seepipeRunner, PipeRunner, pipe runner

TERRA 400 PRM power source

ParameterValue
Current range3 to 400 A
MIG/MAG duty cycle at 40 °C400 A at 50%, 360 A at 60%, 340 A at 100%
Mains supply3 x 400 V ±15%
Power22 kVA
Fuse30 A
Protection ratingIP23S
Weight22.5 kg
Dimensions620 x 240 x 460 mm
Generator operationyes

Which pipes and materials pipeRunner welds

Diameters and wall thicknesses

The smallest pipe is 8 in, which is 219.1 mm. The manufacturer gives no upper limit. You order the band for a specific nominal diameter, so 3 diameters on site mean 3 bands. Inches give the nominal pipe size and millimetres the outside diameter.

Trials with known results:

PipeMaterialWho ran the trial
36 in (914 mm) x 15 mmX70Böhler Welding
24 in (610 mm) x 25 mmX60Böhler Welding
below 20 in, wall 20 to 25 mmX65 clad with alloy 625Böhler Welding
dimensions not given in the sourceaustenitic steel 304LBöhler Welding
Ø610 x 17.5 mmL485MESpawlab with a customer and the manufacturer, first trial in Poland

The published trials cover wall thicknesses from 15 to 25 mm. We found no published manufacturer results for thicker walls, hydrogen pipelines or offshore work. If your project falls outside this range, start with a procedure trial.

Steel grades

Pipe materialWire for fill and cap passes
X60 (L415)diamondspark X60 RC-Pipe
X70 (L485)diamondspark X70 RC-Pipe
X70 for sour servicediamondspark X70 RC-Pipe (N)
X80 (L555)diamondspark X80 RC-Pipe
Pipe clad with alloy 625FOXcore 625-T1
Stainless steel 304LFOXcore 308L-T1

You will find the wire classifications and the root electrodes further down, in the chapter on parameters. If your grade is not in the table, write to us. We will discuss wire selection during the application review.

What pipeRunner does not do

  • It does not weld pipe below 8 in.
  • In the standard procedure it does not lay the root pass. The manufacturer allows downhill MAG (GMAW) welding, for example for the root, but has not published parameters for it.
  • The manufacturer lists no automatic seam tracking function, so assume that the operator keeps the torch on the groove centre line.

Welding step by step, from bevel to cap

The sequence is the same as in our video from the first trial in Poland. Only the step numbers differ. Steps 1, 2, 3, 5, 6 and 7 each link to the relevant point in the video.

Step 1. Prepare the joint and weld the root

In our trial the joint had a 60° V groove, and a welder had laid the root beforehand by TIG. On your job, take the groove shape and the root process from the WPS. The welder lays the root and hot pass by hand, as in your current procedure. After the hot pass, remove the slag and level the profile with a grinder. The first pass from the carriage then has an even base around the whole circumference. Video from 1:45: the 24 in (Ø610 mm) pipe, 60° V bevel and the hybrid method.

Step 2. Fit the band

  1. Clean mud and spatter off the pipe surface where the band will sit.
  2. Fit the band next to the joint. Measure its distance from the groove centre line at 4 points: 12, 3, 6 and 9 o'clock. The distance must be the same all the way round. Take the value from the manual for your kit.
  3. Set the band lock at the top of the pipe, near 12 o'clock, unless the kit manual says otherwise.
  4. Close the lever and check by hand that the band does not move on the pipe.

If the band sits out of square, the torch drifts off the groove centre line. The operator then has to correct it for the whole pass. Video from 2:47: fitting the band.

Step 3. Mount the carriage and set the torch

  1. Mount the carriage on the band and lock it as the kit manual describes.
  2. Set the torch on the groove centre line, at about 90° to the pipe surface.
  3. Set a wire stick-out of 15 to 20 mm.
  4. Fit U-groove feed rolls, because you are welding with flux-cored wire. Set the roll pressure so that the wire does not slip but is not crushed.
  5. Set a gas flow of 15 to 25 l/min.
  6. Route the cables with slack so that they do not pull on the carriage.

Video from 3:31: setting up the carriage, torch and remote control. For set-up details, see pipeRunner: fitting the guide band and setting up the carriage.

Step 4. Check the program and do a dry run

You build the program beforehand in the PC application. Each pass has its own travel speed, oscillation width and oscillation speed. Before you strike the arc, run the carriage over one full half of the pipe without welding. Watch 2 things: whether the torch stays on the groove centre line and whether the cables pull tight anywhere.

Step 5. Weld the fill passes uphill

You start at 6 o'clock and travel to 12 o'clock. In our trial the first pass from the carriage started at 210 A and 22 V. You walk with the carriage, watch the weld pool and adjust the settings with the remote control if needed. The kit manual gives the adjustment range. At 12 o'clock you end the pass, bring the carriage back down and weld the second half in the opposite direction. Offset the start of each pass from the previous one, so that the starts do not sit on top of each other. On the Ø610 mm pipe one fill pass took about 9 minutes. Video from 4:42: start at 210 A and 22 V and from 5:58: fill, about 9 minutes per pass.

Step 6. Remove the slag and inspect the pass

In our trial there was no grinding between passes. Running a hammer lightly along the pass was enough to remove the slag. After each pass, inspect both groove edges and the start and stop points at 6 and 12 o'clock. Grind out an uneven start or a crater before the next pass. Keep to the interpass temperature in your WPS. Video from 5:29: slag removal without grinding.

Step 7. Weld the cap

You weld the cap with the same wire and wider oscillation, so that the pass covers both groove edges. In the manufacturer's trial on 36 in x 15 mm pipe the whole joint had 7 passes. These were the root, the hot pass, and the fill and cap passes from the carriage. Video from 6:45: cap pass.

Step 8. Remove the carriage and move the band

Unlock the carriage as the manual describes, take it off, open the band lever and move the kit to the next joint. The finished joint goes through visual inspection and non-destructive testing to the extent your project requires.

We describe the whole trial in Böhler pipeRunner trial: welding a 610 mm (24 in) pipe.

Parameters, wires and gases for pipeRunner

Parameters from trials

ApplicationCurrentVoltageTravel speed or pass timePreheat and interpass temperatureSource
L485ME steel, Ø610 x 17.5 mm pipe, diamondspark X70 RC-Pipe wire 1.2 mm, M21 gas210 A at the start22 Vabout 9 minutes per passas per the WPSSpawlab trial
X65 pipe clad with alloy 625150 to 180 A23 to 26 V18 to 24 cm/min80 °C and 150 °CBöhler Welding
Stainless steel 304L150 to 180 A18 to 22 V20 to 24 cm/min50 °C and 150 °CBöhler Welding

Common settings from the manufacturer's data:

  • gas flow 15 to 25 l/min,
  • wire stick-out 15 to 20 mm,
  • arc length 3 to 5 mm,
  • torch at about 90°,
  • U-groove feed rolls.

These are starting values from specific trials. Your parameters come from a WPS qualified on your material and your wall thickness.

Wires and electrodes

Pipe materialRoot passHot passFill and cap passesAWS wire classification
X60 (L415)FOX CEL (E6010)FOX CEL 80-P (E8010-P1)diamondspark X60 RC-Pipe, 1.2 mmE81T1-Ni1M-JH4
X70 (L485)FOX CEL (E6010)FOX CEL 80-P (E8010-P1)diamondspark X70 RC-Pipe, 1.2 mmE91T1-K2M-JH4
X70 for sour serviceas per the WPSas per the WPSdiamondspark X70 RC-Pipe (N), 1.2 mmE91T1-GM-JH4
X80 (L555)as per the WPSas per the WPSdiamondspark X80 RC-Pipe, 1.2 mmE101T1-K2M-JH4
X65 clad with alloy 625TIG, UTP A 6222Mo-3 rod, 2.4 mmas per the WPSFOXcore 625-T1see the wire data sheet
Stainless steel 304LTIG, Thermanit JE-308 L rodas per the WPSFOXcore 308L-T1see the wire data sheet

Shielding gas

With diamondspark RC-Pipe wires you use M21 shielding gas, which is argon with 15 to 25% CO2. You weld a TIG root under argon. For FOXcore wires, take the gas from the wire data sheet.

Impact toughness in the manufacturer's trials

In the Böhler Welding trials, the average impact energy was 46 to 85 J at -30 °C. At -60 °C it was 33 to 50 J. These figures apply to the pipes and wires in those trials.

Ask about Böhler wires, rods and electrodes on our Böhler Welding at Spawlab page.

How much time pipeRunner saves

Manufacturer's trial: 66 minutes instead of 109

Böhler Welding compared 2 procedures on the same pipe: X70, 36 in (914 mm) x 15 mm.

MeasurementCellulosic electrode for the whole jointRoot by hand, the rest with pipeRunnerDifference
Total joint time109 min66 min43 min, about 39% less
Arc time71 min 42 s48 min 25 sabout 32% less
Filler metal used3.7 kg2.02 kgabout 45% less
Number of passes1073 fewer

In the manufacturer's materials you will see a claim of 66% time savings. Its own measurements give 66 minutes instead of 109, which is about 39% shorter. Use 66 and 109 minutes in your calculations. The result comes from one trial on one pipe.

Time for one pass by diameter

The arc time for one pass is the pipe circumference divided by the travel speed. The table uses the full circumference, that is, both halves, for speeds of 18 to 24 cm/min.

Pipe diameterCircumferenceTime for one pass
8 in (219.1 mm)688 mm2.9 to 3.8 min
12 in (323.9 mm)1,018 mm4.2 to 5.7 min
16 in (406.4 mm)1,277 mm5.3 to 7.1 min
20 in (508 mm)1,596 mm6.6 to 8.9 min
24 in (610 mm)1,916 mm8.0 to 10.6 min
36 in (914 mm)2,871 mm12.0 to 16.0 min
48 in (1,219 mm)3,830 mm16.0 to 21.3 min

The manufacturer gave the range of 18 to 24 cm/min for pipe clad with alloy 625. In our trial on L485ME steel, one fill pass on the Ø610 mm pipe took about 9 minutes.

What else goes into the calculation

  • moving the band and carriage between joints,
  • changing the 5 kg spool,
  • slag removal and inspection after each pass,
  • waiting for the interpass temperature.

You can work out your own case in the joint calculator on the system page. If you prefer figures from your own pipe, book a trial.

When pipeRunner pays off and when to choose another method

The table shows which jobs suit the pipeRunner carriage and where another method is the better choice.

Your situationVerdictWhy
Field joints and tie-ins on pipelines from 8 insuitablethe carriage weighs 14 kg and runs on a band fitted to the outside of the pipe
Pipe-to-elbow jointssuitableyou can mount the carriage on either side of the band, so you fit the band on the straight pipe section
Process pipework and prefabrication from 8 insuitablerepeat diameters, the same program on successive joints
Your crew welds the whole joint with cellulosic electrodes todaysuitableroot and hot pass stay as they are; you mechanise the fill and cap passes
Clad and stainless pipe from 8 insuitable after a trialthe manufacturer has parameters for alloy 625 and 304L steel
Long, large-diameter transmission pipeline built by a mainline spreadchoose another systemsystems with an internal line-up clamp and several heads welding downhill give more joints per shift
Pipe below 8 innot suitablethis is below the minimum diameter for the carriage
Working in wind without a tentnot suitablewind blows the shielding gas away, and AWS D1.1 allows wind up to 8 km/h for gas-shielded processes
A few joints a yearcheck the costs carefullythe cost of the kit and of procedure qualification is spread over a small number of joints
Hydrogen pipelines, offshore work, wall above 25 mmstart with a trialwe found no published manufacturer results for these applications

How to prepare the site for the carriage

  • Leave enough clear pipe on one side of the joint to fit the band.
  • Give the operator access all round the pipe, including underneath, because the pass starts at 6 o'clock.
  • Put up a tent or windbreaks.
  • Provide a 3 x 400 V supply for the power source and 230 V for the carriage power supply, or bring a generator.
  • Place the power source within cable reach, that is, up to 20 m from the joint.

In the video we explain when not to buy pipeRunner (from 8:04) and how to prepare the site for the carriage (from 9:01).

Common mistakes when welding with an orbital carriage

These mistakes are typical of uphill flux-cored welding with a carriage that runs on a band. The table gives the effect of each mistake and how to avoid it.

MistakeEffectHow to avoid it
Band fitted out of square to the jointthe torch drifts off the groove centre line, lack of sidewall fusion on one sidemeasure the distance from the band to the groove centre line at 4 points
Uneven hot pass and slag left by the electrodelack of fusion and slag inclusions in the first pass from the carriagegrind the hot pass to an even profile
Wire stick-out too longunstable arc, porositykeep it at 15 to 20 mm and correct the torch height
Oscillation too narrowlack of sidewall fusionmatch the width to the groove on every pass, because a V groove widens towards the cap
Wind, or a draught through the pipeporositytent, windbreaks and capped pipe ends
V-groove rolls and high pressurecrushed flux-cored wire, uneven feedingU-groove rolls and only enough pressure to stop the wire slipping
Cables pulling on the carriageuneven travel speed, varying pass thicknessa dry run before each half
Pass starts and stops always in the same placeimperfections at 6 and 12 o'clockgrind the start and the crater, offset the start of the next pass
Interpass temperature too highlower impact toughnessmeasure the temperature before each pass and keep to the WPS limit
Parameters from someone else's trial instead of your own WPSa joint not covered by the qualificationtreat the figures in this guide as a starting point for a trial

The operator watches the weld pool and corrects the torch throughout the pass. To run the carriage, choose someone who knows manual flux-cored welding.

Standards for qualifying procedures and operators

When you switch from electrodes to flux-cored wire on a carriage, you change the welding process and the degree of mechanisation. Your current WPS does not cover this. You need a new procedure qualification and a qualification for the operator.

What you qualifyStandardWhat it means in practice
Welding procedureEN ISO 15614-1pWPS, test piece, testing, the WPQR and, on that basis, the WPS. A joint with the root in process 111 and the fill in process 136 is qualified as a multi-process procedure
Gas pipeline weldingEN 12732requirements for welding steel pipework in gas infrastructure
Pipeline to the client's specificationAPI 1104 or ISO 13847you apply it when the project requires it
Carriage operatorEN ISO 14732qualification test for welding operators in mechanised welding
Welder for the root and hot passEN ISO 9606-1the same qualification as before

Order of work

  1. Collect the project requirements: acceptance standard, steel grade, diameter, wall thickness and impact test temperature.
  2. Write the pWPS. Take the starting parameters from the trials described above.
  3. Weld a test piece on your own pipe. Before that, you can book a trial with us on the same pipe, with the scope agreed before we travel.
  4. Commission the tests and collect the WPQR.
  5. Train the operators and register them for the test to EN ISO 14732.

Böhler Welding states that its team of welding engineers, weldTECH Application Services, supports pipeline contractors.

More on standards in our guides:

Daily operation and maintenance

On site the carriage picks up mud, dust and spatter. Go through the lists below before and after each shift.

Before the shift

  • Check that the band is clean, free of spatter and dents, and that the lever closes firmly.
  • Inspect the torch. The contact tip must not have a worn bore and the gas nozzle must be free of spatter.
  • Clean the U-groove rolls and check that the wire runs through without resistance.
  • Measure the gas flow at the nozzle. It should be 15 to 25 l/min.
  • Tighten and dry the connectors on the control cable and the welding cable.
  • Select the program for your diameter and wall thickness and check it with a dry run.

After the shift

  • Blow off the dust and remove spatter from the carriage. The kit manual shows the points to clean.
  • Wipe the band and put it away so that it cannot deform.
  • Store the carriage in its transport case.
  • Protect the wire spool from mud and water.

What wears on the band

The band is designed so that the guides wear slowly. The spacer balls wear first, and they are the cheapest part of the band.

Troubleshooting

If the carriage does not respond, check the cables and the power supply as the kit manual describes. If that does not help, call us. Spawlab is an authorised Böhler Welding service centre in Poland. We handle repairs and parts at our workshop in Krotoszyn. Report a fault through the service form.

pipeRunner videos from our YouTube channel

We recorded all 4 videos during the first pipeRunner trial in Poland. You will find them on the Spawlab YouTube channel.

VideoLengthWhat you will see
Automated Pipe Welding | Böhler pipeRunner on a 610 mm Steel Pipe10 min 20 snarrated video in English: joint preparation, fitting the band, setting up the carriage, fill passes and cap
Trial video without narration2 min 3 s4K video without narration: joint preparation, root, fill passes and cap
Short: striking the arc55 sarc start, pipe welding and the power source readings
Short: the carriage on the move1 minthe carriage runs on the band, the torch follows the joint

The narrated video minute by minute

Click a time in the table to jump to that part of the video.

TimeWhat you will see
0:46system data and equipment
1:4524 in (Ø610 mm) pipe, 60° V bevel and the hybrid method
2:47fitting the band
3:31setting up the carriage, torch and remote control
4:42start at 210 A and 22 V
5:29slag removal without grinding
5:58fill, about 9 minutes per pass
6:45cap pass
7:19manufacturer's trial: 66 minutes instead of 109
8:04when not to buy pipeRunner
8:23where pipeRunner makes sense
9:01preparing the site for the carriage

Fitting the band and setting up the carriage

A separate page with a video on preparing the system for use: pipeRunner: fitting the guide band and setting up the carriage.

Spawlab channel on YouTube

We publish more trial videos on our channel. Subscribe and turn on notifications if you want to hear about the next video.

Price, delivery and working with Spawlab

Price and purchase terms

ItemValue
Base configuration price53,318.21 EUR net, 65,581.40 EUR gross with 23% Polish VAT. 0% VAT for EU companies with a valid EU VAT number
Leasingavailable in Poland
Deliverywithin 30 working days of order
Warrantymanufacturer's warranty
ServiceSpawlab, authorised Böhler Welding service centre in Poland

Check the current price and availability on the Böhler pipeRunner product page.

How we work together

  1. Application review. You give us the diameters, wall thicknesses, steel grade and number of joints. We check whether the carriage suits your joints, and we tell you in writing if it does not.
  2. Configuration. Bands for your diameters, and a power source, torch and wire for your material.
  3. Quote and preparation for start-up. You receive a quote that lists the kit contents, and we agree the scope of operator training together.
  4. After-sales support. Service and parts are available from Spawlab in Krotoszyn.

Before the quote you can book a trial on your own pipe. We agree the scope before we travel. We ran the first pipeRunner trial in Poland with a customer and the manufacturer, so we know this carriage from hands-on work.

What to send in your enquiry

  • pipe diameters and wall thicknesses,
  • steel grade,
  • number of joints and the schedule,
  • the standard or specification the client uses to accept the joints,
  • the procedure you use today,
  • place of work: site or workshop.

Contact

All pages about this system: pipeRunner system page, product page, customer trials, preparing the system for use and manufacturer's documentation (PDF). You will find other equipment in our welding automation category.

Frequently asked questions about Böhler pipeRunner

Does pipeRunner weld the root pass?

Not in the standard procedure. A welder lays the root with a cellulosic electrode or by TIG. The welder also lays the hot pass, and the carriage welds the fill and cap passes. The manufacturer allows downhill MAG (GMAW) welding, for example for the root, but has not published parameters for it.

What is the minimum pipe diameter for pipeRunner?

The minimum is 8 in, which is 219.1 mm. The manufacturer gives no upper limit. You order the band for a specific nominal diameter.

Does pipeRunner weld pipe-to-elbow joints?

Yes. You can mount the carriage on either side of the band. That lets you fit the band on the straight pipe section next to the elbow.

How long does it take to weld one joint?

In the manufacturer's trial on 36 in x 15 mm pipe the whole joint took 66 minutes. Welded entirely with electrodes, it took 109 minutes. In our trial on Ø610 x 17.5 mm pipe one fill pass took about 9 minutes.

Which wire and gas does pipeRunner use?

For pipeline steels from X60 to X80 you use diamondspark RC-Pipe flux-cored wire, 1.2 mm in diameter, with M21 mixed gas. For pipe clad with alloy 625 you use FOXcore 625-T1 wire, and for 304L steel FOXcore 308L-T1. Choose the gas for FOXcore wires from the wire data sheet.

Do I need to qualify a new welding procedure?

Yes. You change the process and the degree of mechanisation. You need a new procedure qualification to EN ISO 15614-1, or to the standard named in the project, and a new WPS. The root can still be welded with your current process.

What qualification does a pipeRunner operator need?

The carriage operator takes a test to EN ISO 14732. The welder who lays the root and hot pass works under a qualification to EN ISO 9606-1.

Can you weld with pipeRunner in the field?

Yes, under a tent or behind windbreaks, because you weld with shielding gas. The TERRA 400 PRM power source has an IP23S protection rating and can run from a generator.

How much does the carriage weigh and how many people operate it?

The carriage weighs 14 kg without the spool and has 4 handles. An operator works at the joint, and a welder lays the root beforehand.

How does pipeRunner differ from an orbital TIG head?

Closed TIG heads are used for thin-walled, small-diameter tubes. The pipeRunner carriage welds pipe from 8 in by MIG/MAG and runs on a band. The operator controls it with a remote control.

How much does Böhler pipeRunner cost?

The base configuration costs 53,318.21 EUR net, which is 65,581.40 EUR gross with 23% Polish VAT. Leasing is available in Poland. Delivery takes up to 30 working days from order.

Can I see pipeRunner on my own pipe before I buy?

Yes. Book a trial through the form on the trials page or call +48 669 162 833. We agree the scope of the trial before we travel.